Workshop, tools and materials › Lesson 10 of 18 · 11 min read
Joining: soft solder, silver solder, riveting and pinning
Clock parts are joined in four main ways: soldering (soft or hard), riveting, pinning, and threads. This lesson covers the first three. Threaded joints have their own lesson. The aim in every case is a joint that is as strong as the job demands, can be undone if it ought to be, and does no damage to the surrounding metal.
Soldering: the principle
Soldering joins metals with a filler metal that melts at a lower temperature than the parts. The filler does not melt the parts; it wets them and flows into the gap by capillary action, and on cooling forms a thin alloyed layer. Three conditions must be met: clean metal (no oxide, oil or dirt), a flux to keep the joint free of oxide while it heats, and heat on the work, not on the solder alone. Solder flows towards the hottest part of a joint; if you heat the parts, the solder follows.
Fluxes
| Flux type | Used for | Notes |
|---|---|---|
| Rosin (resin) flux | Soft soldering of clean brass and copper | Mild and non-corrosive as a residue; HSE warns that rosin (colophony) fume can cause asthma and dermatitis, so use fume extraction and keep your face out of the fume |
| Zinc chloride ("killed spirits") and similar acid fluxes | Steel and badly oxidised metals | Active and corrosive; residues continue to attack metal, so wash thoroughly and neutralise; avoid on movements wherever you can |
| Phosphoric-acid-based fluxes | Steel, stainless steel | Corrosive; clean thoroughly afterward |
| Borax-based (white) flux | Silver soldering and brazing | Water-soluble paste or powder; glassy residue after heating; dissolve in hot water or pickle |
| Fluoride-containing silver-solder flux | Silver soldering stainless steel or low-temperature work | Read the manufacturer's safety data sheet for the fume hazard of the particular product; ventilate or extract accordingly |
A flux is not a cleaning agent for dirt. Clean the joint first with a file, abrasive paper or a fibre brush, then degrease.
Soft soldering
Soft solders melt below about 450 °C. Traditional tin-lead solders (60% tin, 40% lead) melt over about 183-190 °C according to Kester's alloy chart. Lead-free solders melt a little higher: 217-220 °C for the tin-silver-copper alloy SAC305 and 227 °C for tin with 0.7% copper (same chart); they are generally less free-flowing. They need better temperature control and good flux. HSE lists soldering with lead alloys among the activities with a higher risk of lead exposure, through breathing fume or swallowing lead from unwashed hands, so prefer lead-free solder where the joint allows, wash your hands and face before eating or drinking, and do not eat at the bench (see the safety lesson). Which solder suits a given repair is a matter of typical practice, varies.
Tinning
Tinning means coating the surface with a thin layer of solder before joining. It lets you join parts more reliably, because each surface is already wetted.
- Clean both surfaces to bright metal; handle by the edges.
- Apply a small amount of flux.
- Heat the part (not the solder) with a soldering iron or a small flame; touch the solder to the heated metal so it flows out into a thin, bright layer.
- Wipe off any excess with a clean rag or brush while it is molten.
- Bring the tinned surfaces together, reheat, and hold still until the solder solidifies. Do not move the joint while it cools; a disturbed joint is weak and grainy.
- Clean off flux residues with hot water, a brush, and a neutral wash, then dry.
Choose a soldering iron of enough power to heat the whole part quickly (60-100 W or more for clock work; an electronics iron may not have the thermal mass). A small flame is better for larger parts. Use a heat sink (a pair of tweezers or a damp rag) to protect nearby parts or joints.
Typical clock uses
- Repairing a cracked or loose collet on a wheel.
- Mending a broken spoke or a cracked rim on a wheel (together with a fillet or a brass patch).
- Fixing hammer heads, levers, and similar loose parts.
- Replacing a lost section of a brass part with a built-up repair (soft solder can fill a small gap, but a mechanical repair is preferred where strength matters).
Silver soldering and brazing
Silver solder (strictly, silver brazing alloy) is an alloy of silver, copper, zinc, and sometimes tin, that melts roughly between 600 and 800 °C depending on grade. It gives a joint much stronger than soft solder and can take moderate heat, so it is used where structural strength is needed. The melting figures for silver solder and brazing in this lesson are typical practice, varies with the grade and the maker's data.
| Grade | Approximate melting range | Typical use |
|---|---|---|
| Hard | About 730-790 °C | First joint on a multi-joint job |
| Medium | About 700-760 °C | Second joint |
| Easy | About 690-740 °C | Third joint, small parts |
| Extra-easy (low temperature) | About 620-700 °C | Final joints, thin parts |
The ranges above are approximate and vary with the alloy; check the maker's data sheet. The point of grading is step soldering: make the first joint with the highest-melting grade, then later joints with lower grades, so earlier joints do not melt.
Cadmium
Many older silver solders, especially the lower-temperature "easy-flow" types, contained cadmium. The UK Health and Safety Executive's guidance (EIS31) states that cadmium-bearing silver solders typically contain 16 to 25% cadmium, that heating them above cadmium's 320 °C melting point produces cadmium oxide fume, and that this can cause lung damage hours or days after exposure (sometimes fatal at high exposure) and, with repeated exposure, irreversible kidney damage. HSE says substitution should be considered first and that cadmium-free silver solders are widely available. HSE gives no way to identify an unmarked solder by sight, so if you have an old stick with no marking, ask the supplier or treat it as cadmium-bearing and do not use it. Never overheat silver solder until it fumes; if it does, stop and ventilate.
Procedure
- Fit the joint with a close gap, about 0.05-0.15 mm. Capillary flow works only in a narrow gap.
- Clean by filing or abrasive paper; degrease.
- Flux: paint flux over the joint and the surrounding area.
- Support the work on a firebrick or charcoal block so it is stable and can be heated from below or the side. A binding wire or a clamp holds parts in position.
- Heat gently and evenly with a torch, heating the larger part more. The flux first bubbles, then becomes clear and glassy at the working temperature.
- Touch a small piece of solder (cut into pallions or use a thin wire) to the edge of the joint. It will run into the joint towards the heat. Remove the flame at once.
- Cool in air, then let the flux glass soften in hot water, or use a mild jeweller's pickle (sodium bisulphate crystals in warm water) to dissolve it, then rinse thoroughly. Do not quench red-hot steel parts in water unless you mean to harden them. Wear eye protection and gloves with pickle.
- Clean and finish with files and abrasives.
Brazing with brass filler rod (roughly 850-900 °C) gives a stronger joint than silver solder but needs more heat, and may anneal the parts. In clock work, silver solder is the usual choice.
Heat affects the parts. Brass annealed by silver soldering will be soft; steel parts heated to red and cooled in air may lose temper or distort. Plan the order of work so that heat treatment comes after soldering whenever possible.
Repairing a mainspring end
Traditional carbon-steel mainsprings can be refitted with a new hooking eye. The spring is hard and brittle, and to work the end you must soften it first. Only the end is softened; the rest of the spring stays spring-hard.
- Wear eye protection and gloves, and make sure the spring is fully let down and held in a winder or clamp. Mainsprings store a lot of energy and can lash out.
- Cut or snap off the broken end, leaving a clean end.
- Heat the end of the spring (the last 20-30 mm is typical practice, varies) to a dull red and let it cool slowly. This softens it (annealing, essentially tempering the hardened steel right back down).
- Mark the position of the new hole or hook, drill with a small drill or punch the hole, and file the end so it is square and smooth.
- Fit the spring and check that the eye engages the barrel hook and does not tear. The softened end is left as it is; the rest of the spring remains spring-hard.
Modern stainless and alloy springs cannot be softened and reworked in this way. Replace them, or have the spring made to length by the supplier.
Riveting and peening
A rivet holds two parts by a head at each end. Clock riveting is the permanent attachment of wheels to collets and pinions, pillars to plates, and bushes in some cases. Peening is working metal by hammering, usually to spread it.
Riveting a wheel to its collet
- Chamfer the hole or the collet seat slightly to make a lip that will roll over.
- Seat the wheel on the collet, square and centred. Check that the wheel runs true by spinning it on the arbor.
- Support the work on a hole in the stake that clears the arbor and supports the collet.
- Use a hollow rivet setter (rounding-up punch) that fits over the collet. Strike it with the hammer lightly and rotate the punch between blows so the lip spreads evenly all round.
- Check the wheel for flatness and concentricity; correct any distortion before it gets worse.
Take care not to over-peen: hammering work-hardens the metal and it will crack. Use a smaller hammer and more blows rather than a large hammer and few. Brass is best peened without annealing for clock work; annealed brass is too soft to hold.
Riveting pillars
On many clocks the pillars are riveted to the front plate and held on the back plate by taper pins. To remove a riveted pillar, file or drill the rivet end, then drive it out; to re-rivet, support the plate against a flat stake and peen the tenon with a ball-pein hammer, working round the tenon and avoiding hammering the plate surface.
Taper pins and clock pins
Taper pins locate and hold parts such as plates, hands, collets and cannons, and can be pulled out easily. A taper pin is a tapered rod pressed into a matching tapered hole, and the friction of the wedge holds it. Engineering taper pins have a standard taper (about 1:50 for metric pins, as in ISO 2339, and about 1:48 for inch pins) and are fitted to reamed holes. Clock pins are a clockmaker's older form: I found no universal standard for them; they are usually steeper in taper than engineering pins, and the holes are typically cut with a clockmaker's cutting broach instead of a reamer (typical practice, varies). Suppliers number their own ranges, so sets from different makers are not interchangeable. What matters is having a range of sizes (see the lesson on taper pins in practice).
Fitting a taper pin
- Broach the hole until the pin enters about two thirds of its length by hand pressure.
- Tap it home with a light hammer, supporting the work from behind.
- Cut or file the long end; leave about as much length protruding as the hole diameter, and file the end smooth.
- Re-use pins only if they are straight and unmarked.
Use a pin punch to drive a pin out from the small end. A pin that will not come out is likely corroded in place: apply a little penetrating oil, tap sideways to break the bond, and avoid large forces on the plate. If a pin is stuck, drilling it out is better than levering.
Making your own pins
Put a length of steel or brass wire in a pin chuck, rest it on a wooden block, roll it with one hand and file across it at a slight angle, so it takes a taper. Match the angle of the pin to the broach by trying it in the hole.
Steel pins in brass holes
This is an unsettled debate. Some makers avoid putting steel pins in brass holes, and some always do it without trouble; see the article on this. Whichever you choose, keep a variety of pins in stock and always make the pin small enough that it can be replaced.
Common mistakes
- Soldering without cleaning, then blaming the solder.
- Heating the solder instead of the work, which gives a blob that does not flow.
- Leaving acid flux residue on a movement, which corrodes it over months.
- Hammering a taper pin so hard that the plate distorts or cracks.
- Over-peening a rivet and cracking the collet.
Sources
- Exposure to cadmium in silver soldering or brazing, EIS31 (HSE)
- Solder fume and you, INDG248 (HSE)
- Working safely with lead: when are you most at risk? (HSE)
- Alloy temperature chart (Kester, solder manufacturer)
- ISO 2339:1986 Taper pins, unhardened (ISO)
Silver solder and brazing temperatures, procedures and riveting methods are typical workshop practice and vary; I found no single published standard I could read for them.
Get new lessons by email
Free, practical clock repair lessons for beginners. No spam, unsubscribe any time.