Workshop, tools and materials › Lesson 15 of 18 · 19 min read
Hardening and tempering silver steel and gauge plate
The general lesson on heat treatment explains what happens inside steel. This lesson is the working manual for the two steels you will actually harden: silver steel (round bar) and gauge plate (ground flat stock). It gives the temperatures the steelmakers publish, explains why one is quenched in water and the other in oil, and takes you through three complete jobs. Furnace temperatures and hardness figures below come from the steelmakers' own data sheets; colour-based figures (heat colours and oxide colours) are approximate workshop guides and are marked as typical practice, varies.
The two steels
| Silver steel | Gauge plate | |
|---|---|---|
| Form | Bright ground round bar, imperial and metric | Precision ground flat bar and sheet, flat and square to close tolerance |
| Specification | BS 1407 (published by BSI in 1970 and still listed as current; the name is still used by suppliers) | Sold as O1 oil-hardening tool steel or an equivalent grade (O1 is 1.2510 / 100MnCrW4 in the European system) |
| Carbon | 0.95-1.20 % (Erasteel data sheet) | about 0.85-1.0 % (Industeel) |
| Other elements | chromium 0.35-0.45 %, manganese 0.25-0.45 % (Erasteel) | manganese about 1.2 %, chromium about 0.5 %, tungsten about 0.5 %, vanadium about 0.1-0.2 % (Industeel, Carpenter) |
| Hardening type | Water-hardening (the W1 family in American terms) | Oil-hardening |
| Hardness as supplied | Erasteel gives an approximate Brinell range of 180-285 as supplied (guidance only) | soft enough to file and drill; about 217 HB maximum when annealed |
| Best for | Pivot files, punches, drills, broaches, arbors, small cutters, pins | Pallets, anvils, stakes, flat gauges, templates, cutters that must stay flat |
Silver steel is named for its bright surface; there is no silver in it. Its carbon content is close to 1 %, which is why a small piece quenched correctly reaches about 64-66 HRC (Rockwell C, the usual hardness scale for hard steel). American water-hardening tool steels (the W1 family) are similar in carbon but not identical in the minor elements, so for silver steel use the data sheet of the actual silver steel where you can.
Gauge plate owes its different behaviour to manganese, chromium and tungsten. These elements slow the transformation back to soft structures during cooling, so the steel hardens right through in oil, a much gentler quench than water. The same alloying makes gauge plate move less when hardened, which is why it is the material for anything that has to stay flat.
Heat colours: judging temperature by eye
A workshop has no furnace thermometer, so hardening is judged by colour. The colour of red-hot steel depends on temperature, but also on the lighting, on your eyes and on the surface, so treat the values below as approximate. Published colour tables disagree by tens of degrees, and We did not find a single authoritative standard for them, so the table below is typical practice and varies. Judge in subdued, constant light rather than bright sun, because in sunlight a piece at the right temperature looks darker than it is.
| Appearance in subdued light | Approximate temperature (typical practice, varies) | Use |
|---|---|---|
| First dull glow, only visible in the dark | about 525-600 °C | Too cool for anything but stress relief |
| Dull red | about 700 °C | Just under the hardening range |
| Dull cherry red | about 770-800 °C | Hardening range for silver steel and gauge plate |
| Full cherry red | about 850-900 °C | Too hot for these steels; grain coarsens and carbon is lost |
| Orange to yellow | about 1000-1250 °C | Forging heat; far too hot for clock steel |
| White | 1300 °C and above | Burning; the steel is ruined |
A second, independent check is the magnet. Iron loses its attraction to a magnet at its Curie temperature of about 770 °C (a standard physics value; steel with carbon and alloying elements loses it at similar temperatures), which is close to the hardening temperature of silver steel, so a piece held in tongs that a small magnet on a stick will no longer pick up has reached roughly that temperature. Use the colour and the magnet together, not either alone, and do not hold the magnet in the flame.
Hardening temperatures
| Steel and source | Austenitising (hardening) temperature | Quench |
|---|---|---|
| Silver steel (Erasteel STUBS data sheet) | 770-790 °C for maximum hardness (66 HRC) | Clean water or, preferably, 10 % brine |
| Related grade 1.2210 / 115CrV3 bar (ArcelorMittal OMMIS data sheet) | 810-840 °C under 15 mm diameter; 780-810 °C over 15 mm | Oil under 15 mm; water over 15 mm (64 HRC as quenched) |
| O1 / gauge plate (Carpenter) | 788-816 °C | Oil |
| O1 / gauge plate (Industeel data sheet) | 780-820 °C, preheat to about 650 °C | Warm (about 55 °C), thin, agitated oil |
| O1 / gauge plate (Uddeholm Arne data sheet) | 790-850 °C, preheat 600-700 °C | Oil (about 64-65 HRC as quenched) |
For the bench, aim for the middle of these windows: about 780 °C for silver steel and about 800 °C for gauge plate. Both are an even dull cherry red with the colour uniform right through the section. Colour is a loose guide, so use your magnet and your test pieces to calibrate your eye. Note that ArcelorMittal's data sheet for a related chromium-vanadium bar steel specifies oil for small diameters, a reminder that the quench for silver steel is a judgement about section size and cracking risk.
Soak. Industrial data sheets specify soaks of roughly 15 to 30 minutes after the load reaches temperature (Industeel, Uddeholm) because they heat whole furnace loads. At the bench, once the piece is uniformly at colour, hold it there for about a minute for a 6 mm section, a little less for smaller; this is typical practice, varies, and there is no published figure for torch heating. Longer soaking does nothing useful with a torch and only invites scale and decarburisation.
Quench media: why water for silver steel and oil for gauge plate
Hardening needs the steel to cool from red heat past the "nose" of its transformation curve fast enough that it turns into martensite instead of soft pearlite. A plain carbon steel such as silver steel has little alloy to slow that transformation, so it needs a very fast quench; water or brine does it. The alloys in gauge plate slow the transformation, so oil, which cools much more gently, is fast enough.
| Quenchant | Cooling speed | Notes |
|---|---|---|
| 10 % brine | Fastest | Gives the hardest result on silver steel. Brine corrodes steel, so rinse and dry the part at once. |
| Clean cold water (about 15-20 °C) | Very fast | The standard for silver steel. Agitate, because steam bubbles clinging to the surface insulate it and leave soft spots. |
| Quenching oil, warm | Moderate | The correct choice for gauge plate. Industeel specifies warm, thin, agitated oil at about 55 °C; warm oil is thinner and cools more evenly. |
| Cold oil | Moderate to slow | Works for small parts, and a silver steel part that is quenched in oil may not reach full hardness. |
Quenching silver steel in oil is sometimes done for thin or intricate work, because oil is less likely to crack it. It is a trade: you accept a lower hardness in exchange for a lower risk. Quenching gauge plate in water is not recommended: it is already somewhat prone to cracking even in oil, and water makes that far worse.
Tempering
As quenched, the steel is glass-hard and highly stressed. It may crack on its own, in hours or days, if it is not tempered. Reheating it to a modest temperature relieves some of the stress and trades a little hardness for a great deal of toughness. For O1, Uddeholm says to temper as soon as the part has cooled to 50-70 °C after an oil quench; Erasteel specifies tempering immediately after hardening for silver steel.
Hardness against tempering temperature
The Erasteel data sheet for silver steel gives the following figures for a minimum one-hour soak after hardening at 770-790 °C. Oven tempering gives these values; torch tempering by colour is less precise. ArcelorMittal's data sheet for a related 115CrV3 bar gives 62 HRC at 200 °C and 57 HRC at 300 °C, in the same range.
| Tempering temperature | Hardness (HRC) |
|---|---|
| As quenched | about 66 |
| 150 °C | 63-65 |
| 200 °C | 60-62 |
| 250 °C | 59-61 |
| 300 °C | 55-57 |
Two points are worth noting. The fall in hardness between 150 and 250 °C is small (about 4 HRC), but the gain in toughness is large. Between 250 and 300 °C the hardness drops faster. O1 is about 64 HRC as quenched (Industeel); both Industeel and Uddeholm publish tempering curves, so read the hardness for your chosen temperature from the maker's chart. The Industeel sheet recommends a double temper between 150 and 250 °C, and a minimum of two hours per 25 mm of section; for small clock parts, one hour at temperature followed by a second cycle is a sensible equivalent.
Oxide colours
If you do not have an oven, you can temper by colour. When clean, bright steel is heated in air it forms a thin transparent oxide film. The film is a few hundred nanometres thick at most, and its colour is an interference effect: light reflecting from the top of the film and from the steel beneath interferes, cancelling some wavelengths and reinforcing others. Thicker film means a different colour, and film thickness grows with temperature (and with time), so the colour records the highest temperature reached.
| Colour | Approx. temperature (typical practice, varies) | Typical use (approximate) |
|---|---|---|
| Very pale yellow | about 210-220 °C | Very hard: pivot files, burnishers, scrapers, engraving tools |
| Straw | about 220-230 °C | Lathe tools, hammers, drills for hard use, small punches |
| Dark straw to yellow-brown | about 240-250 °C | Drills, broaches, dies, taps |
| Brown / red-brown | about 250-265 °C | Cold chisels, centre punches, drifts |
| Purple | about 270-280 °C | Screwdrivers, tougher tools |
| Dark blue | about 290-300 °C | Springs, clips, parts that will be bent, pallets that need toughness |
| Light blue | about 310-320 °C | Very tough and soft; no longer a useful tool temper |
| Grey-blue to grey | above about 320-340 °C | Effectively soft; time to start again |
Heed the caveats. The colour-to-temperature pairings above are workshop convention; We did not find them in a standard, and published charts differ. The colour order itself is well established (the US National Bureau of Standards lists light straw, straw, dark straw, brown, purple, dark blue and light blue in order of increasing film thickness) and depends on time as well as temperature: the same source says blue can form anywhere between roughly 260 and 370 °C, taking about an hour at the low end and about a minute at the high end. Surface finish matters (polished steel shows true colours; a scratched or oily surface does not) and alloys may differ. Treat the colour as a guide to the right neighbourhood. The hardness table above was measured at fixed temperatures in a furnace and is the more reliable guide.
Tempered martensite embrittlement is a further reason not to be careless. Cambridge University's materials pages describe it as occurring at about 300-350 °C, where cementite particles coarsen and act like brittle inclusions, so that toughness can fall even though the steel is tempered; other sources quote a somewhat wider range. This is a reason to choose a temper colour deliberately and not let it drift. Springs and other parts conventionally tempered to blue are made from steels intended for that; for ordinary silver steel, if you do not need a spring temper, stay below it.
What temper for what
| Part | Temper | Why |
|---|---|---|
| Pivot file, burnisher, graver for brass | Light straw (about 220 °C) or the minimum that removes stress | Needs maximum edge hardness; a thin tool that is cared for rarely meets shock |
| Punch, centre punch | Straw to brown on the striking end | The tip is hard, the head tougher so it does not shatter |
| Drill, broach, reamer (home made) | Straw to dark straw | Hard enough to cut brass, tough enough to resist chipping |
| Pallets, steel anvils, stakes | Straw (hard wear parts) to blue (impact parts) | Choose by whether wear or breakage is the greater risk |
| Spring, clip, click spring | Dark blue (about 300 °C) | Must flex without taking a set |
| Scraper, glass drill | Left fully hard, or lightly tempered | Wear resistance matters more than toughness |
Remember the temper is a compromise you are making deliberately: a pallet tempered to blue will wear faster than one tempered to straw, but it is less likely to snap. The pairings in the table above are typical practice, varies.
Annealing and spheroidising
Annealing makes steel soft again, either to machine it, to correct a bad hardening, or to drill a hard arbor. Heat to just above the hardening temperature range and cool very slowly. The data sheets are specific for furnace work.
| Steel and source | Anneal at | Cooling | Result |
|---|---|---|---|
| Silver steel (Erasteel) | 760-780 °C | Slowly in the furnace | Brinell 180-285 as supplied (guidance) |
| O1 (Carpenter) | 760-788 °C | Not faster than 11 °C per hour | 217 HB maximum |
| O1 (Industeel) | 750-780 °C | 10-20 °C per hour to 600 °C, then air | 212 HB maximum |
| 115CrV3 bar (ArcelorMittal OMMIS) | 710-750 °C | Not stated in the extract I read | 245 HB maximum in the delivered state |
No clockmaker cools at 10 °C an hour, but you can get close enough: heat the part to dull red, then bury it in a tin of dry vermiculite, dry wood ash or lime so that it takes hours to cool. Burying the hot part in ashes is the traditional method (typical practice, varies). For a quick softening of one end of a hard arbor, heat the end until it turns blue and let it cool in air; this tempers rather than anneals, but it is often enough to let a drill cut. If the part still files hard, anneal properly.
Spheroidising is a prolonged anneal that turns the plate-like carbide in the steel into small spheres, giving the softest and most machinable state of high-carbon steel. It involves holding at or just above the lower critical temperature for several hours, or cycling around it, followed by very slow cooling. A research paper on a chromium high-carbon steel used 8 hours at 790 °C, about 39 °C above that steel's calculated lower critical point (751 °C), followed by furnace cooling to 520 °C. You will rarely need to do this in a clock workshop; bar stock is supplied in an annealed or spheroidised state, and a slow-cooled part is soft enough to work.
Scale and decarburisation
At red heat the steel reacts with air in two ways. It forms scale, a black iron oxide that flakes off and leaves a rough, pitted surface. It also loses surface carbon, which is called decarburisation. A part that has lost its surface carbon will not harden at the surface even though the inside is hard, so a file skates on a freshly ground face but bites in a surface that was not ground. Overheating makes both worse and can stop the steel hardening properly.
- Work to size after hardening, or leave stock. Leave 0.1-0.2 mm of extra material on critical faces and finish by stoning or lapping afterwards. This removes the soft skin. (This allowance is common practice, not a published figure.)
- Keep the heating short. Use a torch that brings the piece to colour quickly, and do not hold it at temperature for longer than the section needs.
- Keep the air out. In a muffle furnace Erasteel specifies a slightly reducing atmosphere; at the bench the equivalent is to wrap the part in stainless steel foil (typical practice, varies), to heat it inside a closed steel tube or box packed with cast-iron chips or charcoal, or to coat it with a hardening flux that forms a thin glaze. Small insulated parts on charcoal are heated this way to avoid burning and decarburising them.
Cracking and distortion
| Cause | Cure |
|---|---|
| Sharp internal corners, holes near edges, stamped numbers | Radius corners, keep holes away from edges, drill and file all marks out before hardening |
| Uneven heating (one side hotter) | Heat slowly and evenly, rotate the work, and heat a heavy section from the heavy side |
| Overheating | Quench at dull cherry, never white or bright orange |
| Thin and thick section together | Heat the thick part first; quench thick end first where you can |
| Wrong quench for the steel | Water for silver steel, oil for gauge plate; use oil for silver steel if the shape is risky |
| Quenching a long piece flat | Quench long rods end-on, vertically, or with a slight spin; use a figure-of-eight motion to avoid vapour pockets and warping |
| Delay before tempering | Temper at once; a quenched part can crack by itself on the shelf |
| Water or oil on the part when it goes to the torch for tempering | Clean and dry first, and brighten the part with emery so the colours show |
Testing with a file
A new, sharp, fine file is the standard hardness test. Clean the part to bare steel (the scale and the soft decarburised skin must be removed, or the test is meaningless) and draw the file lightly across a corner. A part that is properly hard turns the file: it skates and slips and leaves a bright, shiny streak rather than a cutting mark. If the file bites, the steel is not hard enough: the temperature was too low, the quench too slow, the surface decarburised, or the part was tempered after hardening. Once the part is tempered, the file will bite more readily, so do the file test before tempering, on a spare corner, and do not rely on the test to judge temper. Always test on a scrap piece of the same steel hardened alongside the job, because a file used on the finished surface leaves a mark. The test shows only that the steel is hard (roughly above 58-60 HRC, an approximate figure), not how hard.
Worked examples
Temperatures come from the data sheets above; torch heating times, soak times and tempering colours in these examples are typical practice, varies.
Example 1: a pivot file from a short length of 3 mm silver steel
- File or grind the shape and surface finish first; steel is easy to work while soft. Chamfer the corners.
- Prepare a quench container with about 1 litre of clean water at room temperature, and the test scrap (a 20 mm length of the same bar).
- Support the piece on a firebrick in a dim part of the bench. Warm it gently with the torch, moving the flame along its length, then bring it to a dull cherry red (about 780 °C). Bring the scrap to the same colour beside it.
- Test with a magnet on a stick: the steel should be non-magnetic. Hold the colour for about 30 seconds.
- Pick up with tongs and quench vertically, end-first, in one smooth movement. Stir gently up and down for a few seconds. Do not drop the part or take it out of the water until it stops hissing.
- Dry it. Test the scrap with a file: it should skate. If it does, the process worked.
- Polish one face with fine emery so the colours will show. Temper at once. Place the piece on a steel plate or in a pan of brass filings, heat gently from below until the surface turns light straw (about 220 °C), and quench or let cool.
- Clean, check the file edge, and finish.
Example 2: a small clock anchor (pallet) blank from 2 mm gauge plate
- Cut, file and drill to final form, leaving 0.15 mm on the faces that will be finished, and drill the arbor hole. Remove every burr and radius the corners.
- Warm a tin of quenching oil (not engine oil) to about 50 °C in hot water. Lid ready, glasses on.
- Heat evenly to dull cherry (about 800 °C), keeping the flame moving so the thin arms do not overheat before the boss. Hold until colour is even throughout, about 30-60 seconds.
- Quench in the oil with a slight swirl. Leave for a minute, then lift out. The part will be oily and warm.
- Wipe it, test a corner with a file, then without delay clean one face with emery and temper to straw (about 220-230 °C) if it is a wear part, or to the dark straw/purple range if the arms are slender and could snap.
- Stone the faces back to size. Because you left excess, the soft skin is gone.
Example 3: a home-made 1.2 mm cutting broach from silver steel
- File the taper and the five (or four) cutting flats while soft. Leave the working end slightly oversize.
- Harden as in Example 1, quenching vertically and spinning gently. A thin tool should go point-first.
- Temper to dark straw (about 240 °C). Use a small flame at the shank end so the colour runs toward the cutting end, and quench when the working tip reaches a pale straw. The shank end will be softer and tougher, which reduces the chance of the tool snapping at the handle.
- Stone the flats to a sharp edge, test on a brass offcut.
Common mistakes
- Judging colour in bright light and hardening too hot.
- Hardening part of the piece only (the thin end overheats while the thick end is still dull red).
- Quenching, then putting the part in a drawer to temper later.
- Relying on the file to confirm hardness after tempering.
- Using the same temper colour on every job.
- Tempering a part that is oily or scratched, so the colours do not show.
- Re-hardening the same piece more than two or three times, which coarsens the grain and increases decarburisation.
Sources
- Erasteel STUBS Silver Steel data sheet (Erasteel; copy hosted by a distributor)
- BS 1407:1970 Specification for high carbon bright steel (silver steel) (BSI)
- OMMIS 2210 stub (1.2210 / 115CrV3) product datasheet, October 2022 (ArcelorMittal OMMIS)
- O1 data sheet (Carpenter Technology)
- O1 / 2510 data sheet (Industeel ArcelorMittal)
- Uddeholm Arne (O1) data sheet (Uddeholm)
- Oxide on steel and tempering colours (University of Cambridge)
- Bluing of iron and steel, Letter Circular LC630 (US National Bureau of Standards)
- Tempered martensite embrittlement (University of Cambridge)
- Tailoring strength and ductility of a Cr-containing high carbon steel by cold-working and annealing (Materials, 2019, via PubMed Central)
- Used engine oil (HSE)
Get new lessons by email